Acushnet
O-Ring Products
Properties
of Standard Acushnet Compounds
PROPERTIES
|
EPDM's
|
FLUOROCARB0NS
|
E-17016
| E-17018
| F-13667
| F-13664
| F-13329
| F-13681
|
ORIGINAL
PROPERTIES
|
Hardness
Shore"A"
|
70
|
80
|
75
|
75
|
75
|
90
|
Tensile
Strength, p.s.i.
|
1750
| 2000
|
1983
|
1800
| 1775
|
1880
|
Ultimate
Elongation, %
|
200
|
210
|
181
|
175
|
185
| 173
|
ModuIus
@100%, p.s.i.
|
600
|
1000
|
Heat
Aging 70 Hrs. @ 212oF
|
70Hrs. @257oF
|
70Hrs. @482oF
|
Hardness
Change, Points
| +4
|
+3
|
+1
|
+3.5
|
+1
|
+1
|
Tensile
Change, %
| +10.9
|
+23.6
|
-6.6
|
-6.6
|
+10.0
| +5.3
|
Elongation
Change. %
| +8.3
|
+6.7
|
+3.9
|
+2.0
|
-10.0
| -13.9
|
Weight
Loss, %
|
|
|
-1.9
| -0.2
|
-1.5
|
-1.1
|
Compression
Set 70 Hrs.
|
@212oF
| 70Hrs.
@257oF
| 70Hrs.
@392oF
|
%
Set
|
17.3
| 12.0
| 16.1
|
19.3
| 14.2
| 18.5
|
Low
Temperature Flexibility
|
5 Hrs. @ -65oF
|
5
Hrs.@ -40o
|
Pass
| Pass
|
Low
Temperature Retraction
|
TR,
(Point oF)
|
|
| +3
|
+3
|
+3
|
+3
|
ASTM
Fuel B 70 Hrs. @ R T.
|
Hardness
Change, Points
|
|
|
-1
|
-3
| -1
|
-1
|
Tensile
Change, %
|
|
| -6.6
| -6.6
| -3.0
|
-2.6
|
Elongation
Change,
|
|
| -0.6
| -3.0
| -5.0
| -5.8
|
Volume
Change, %
|
|
|
+2.3
| +1.5
| +2.0
| +1.5
|
Ozone
Resistance 500 Hrs.
|
d@
10,000 pphm
20% Extension-Cracking
|
None
|
Weathering
| Excellent
|
Individual
typical physical properties data sheets are available upon
request for these standard and other Acushnet compounds.
|
Contact
us today.
Large Inventory, Fast Service.

|
General Information | Acushnet
O-Ring Products |
|